Tabella 1.Firxiet ta 'kompożizzjoni għal 316 grad ta' azzar li ma jissaddadx.

Grad   C Mn Si P S Cr Mo Ni N
316 Min - - - 0 - 16.0 2.00 10.0 -
Max 0.08 2.0 0.75 0.045 0.03 18.0 3.00 14.0 0.10
316L Min - - - - - 16.0 2.00 10.0 -
Max 0.03 2.0 0.75 0.045 0.03 18.0 3.00 14.0 0.10
316H Min 0.04 0.04 0 - - 16.0 2.00 10.0 -
max 0.10 0.10 0.75 0.045 0.03 18.0 3.00 14.0 -

 

Proprjetajiet Mekkaniċi

Tabella 2.Proprjetajiet mekkaniċi ta 'azzar li ma jissaddadx ta' grad 316.

Grad Tensile Str (MPa) min Rendiment Str 0.2% Prova (MPa) min Tawwal (% f'50 mm) min Ebusija
Rockwell B (HR B) max Brinell (HB) max
316 515 205 40 95 217
316L 485 170 40 95 217
316H 515 205 40 95 217

 

Nota: 316H għandu wkoll rekwiżit għal daqs tal-qamħ ta 'ASTM no. 7 jew aktar oħxon.

Proprjetajiet Fiżiċi

Tabella 3.Proprjetajiet fiżiċi tipiċi għal azzar inossidabbli ta 'grad 316.

Grad Densità (kg/m3) Modulu Elastiku (GPa) Ko{0}}eff medju tal-Espansjoni Termali (µm/m/grad) Konduttività Termali (W/mK) Sħana speċifika 0-100 grad (J/kg.K) Reżistività Elet. (nΩ.m)
0-100 grad 0-315 grad 0-538 grad F'100 grad F'500 grad
316/L/H 8000 193 15.9 16.2 17.5 16.3 21.5 500 740